dc.contributor.advisor | Syafrinani | |
dc.contributor.advisor | Agusnar, Harry | |
dc.contributor.author | Butarbutar, Selamat Suhardi | |
dc.date.accessioned | 2021-04-28T03:31:49Z | |
dc.date.available | 2021-04-28T03:31:49Z | |
dc.date.issued | 2021 | |
dc.identifier.uri | http://repositori.usu.ac.id/handle/123456789/32267 | |
dc.description.abstract | Restorasi sementara dikenal sebagai gigi tiruan cekat sementara yang digunakan
dalam jangka waktu pendek selama restorasi permanen dibuat. Pembuatan restorasi
sementara bertujuan untuk melindungi jaringan oral, estetis dan menjaga fungsi pengunyahan
sampai restorasi permanen dipasang. Tujuan penelitian ini adalah untuk mengetahui pengaruh
penambahan nanopartikel ZrO2 dengan konsentrasi 5% dan 7% pada bahan restorasi
sementara RAPP pada gigi tiruan cekat terhadap kekuatan fleksural dan kekerasan
permukaan. Rancangan penelitian ini adalah eksperimental laboratoris. Penelitian dilakukan
pada sampel bahan restorasi sementara RAPP tanpa penambahan bahan penguat, dengan
penambahan bahan penguat nanopartikel ZrO2 konsentrasi 5% dan 7% dengan ukuran sampel
10 mm x 65 mm x 2,5 mm untuk uji kekuatan fleksural dan sampel ukuran 10 mm x 30 mm x
2,5 mm untuk uji kekerasan permukaan. Jumlah total sampel sebanyak 54 sampel yang terdiri
dari 27 sampel untuk uji kekuatan fleksural dan 27 sampel untuk uji kekerasan permukaan.
Setiap sampel dilakukan pengujian kekuatan fleksural dan kekerasan permukaan dan
kemudian dianalisis dengan uji univarian untuk mengetahui nilai rerata dan standar deviasi
masing–masing kelompok. Uji t-test untuk mengetahui pengaruh penambahan ZrO2 terhadap
kekuatan fleksural dan kekerasan permukaan bahan restorasi sementara RAPP pada gigi
tiruan cekat. Data yang diperoleh normal dan homogen p=0,65 (p>0,05). Hasil penelitian ini
menunjukkan adanya pengaruh penambahan nanopartikel ZrO2 5% dan ZrO2 7% pada bahan
restorasi sementara RAPP gigi tiruan cekat terhadap kekuatan fleksural dan kekerasan
permukaan bahan restorasi sementara RAPP gigi tiruan cekat. Uji kekuatan fleksural pada
restorasi sementara RAPP tanpa penambahan bahan penguat dan RAPP dengan penambahan
ZrO2 5% diperoleh p=0,001; pada restorasi sementara RAPP tanpa penambahan bahan
penguat RAPP dengan penambahan ZrO2 7% diperoleh p=0,001, sehingga dapat terlihat ada
perbedaan yang signifikan pada nilai kekuatan fleksural dari ketiga kelompok. Pada uji
kekerasan permukaan dari restorasi sementara RAPP tanpa penambahan bahan penguat dan
pada RAPP dengan penambahan ZrO2 5% diperoleh p=0,887. Pada uji kekerasan permukaan
dari restorasi sementara RAPP tanpa penambahan bahan penguat dan RAPP dengan
penambahan bahan penguat ZrO2 7% diperoleh p=0,044. Dari hasil penelitian dapat
disimpulkan bahwa penambahan ZrO2 5% dan ZrO2 7% dapat menurunkan kekuatan fleksural
dari restorasi sementara RAPP tetapi dapat meningkatkan nilai kekerasan permukaan
restorasi sementara RAPP dengan bahan penguat ZrO2 dengan konsentrasi 7% sehingga
bahan restorasi sementara RAPP gigi tiruan cekat yang dihasilkan menjadi lebih kuat dan
tidak mudah fraktur dan aus pada saat mendapat beban terutama pada kasus kasus pembuatan
gigi tiruan cekat yang memerlukan proses laboratorium yang lama misalnya gigi tiruan cekat
long span dan gigi tiruan multi-unit. | en_US |
dc.description.abstract | Temporary restorations are known as temporary fixed dentures that are used in the
short term as long as permanent restorations are made. The fabrication of temporary
restorations aims to protect oral tissue, aesthetically and maintain the function of mastication
until a permanent restoration is finished. The purpose of this study was to determine the
effect of adding ZrO2 nanoparticles with concentrations of 5% and 7% to RAPP material of
fixed dentures on flexural strength and surface hardness. The design of this study is an
experimental laboratory. The study was conducted on RAPP temporary restoration material
samples without the addition of reinforcing agents, with the addition of ZrO2 nanoparticle
reinforcement with a concentration of 5% and 7% with a sample size of 10 mm x 65 mm x
2.5 mm for flexural strength test and a sample size of 10 mm x 30 mm x 2.5 mm for surface
hardness testing. The total number of samples was 54 samples consisting of 27 samples for
flexural strength test and 27 samples for surface hardness test. Each sample is tested for
flexural strength and surface hardness and then analyzed with a univariate test to determine
the mean value and standard deviation of each group. T-test to determine the effect of the
addition of ZrO2 on flexural strength and surface hardness of the RAPP on fixed dentures.
The data were normal and homogeneous p = 0.65 (p> 0.05). The results of this study indicate
that there were influence of the addition of 5% ZrO2 nanoparticles and 7% ZrO2 to the
temporary restoration RAPP of fixed dentures on flexural strength and surface hardness of
RAPP temporary restoration material. Flexural strength test on the RAPP temporary
restoration material without the addition of reinforcing material and RAPP temporary
restoration material with the addition of 5% ZrO2, p = 0.001 was obtained; in the RAPP
temporary restoration material without the addition of reinforcement material and RAPP
temporary restoration material with the addition of 7% ZrO2, p = 0.001 was obtained, so there
were significant differences in the flexural strength values of the three groups. In the surface
hardness test of the RAPP temporary restoration material without the addition of reinforcing
materials and on the RAPP temporary restoration material with the addition of 5% ZrO2, p =
0.887 was obtained. In the surface hardness test of the temporary restoration of RAPP
temporary restoration material without the addition of reinforcing material and RAPP
temporary restoration material with the addition of 7% ZrO2, p = 0.044 was obtained. From
the results of the study it can be concluded that the addition of 5% ZrO2 and 7% ZrO2 can
reduce the flexural strength of RAPP temporary restorations but can increase the hardness
value of the RAPP temporary restoration surface with addition of ZrO2 7% so that the
temporary restoration RAPP of fixed dentures becomes stronger and not easy to fracture and
wear when loading especially in cases of fixed denture fabrication which requires a long
laboratory process such as long span and multi-unit fixed denture. | en_US |
dc.language.iso | id | en_US |
dc.publisher | Universitas Sumatera Utara | en_US |
dc.subject | Restorasi sementara | en_US |
dc.subject | Zirkonium Oksida | en_US |
dc.subject | kekuatan fleksural | en_US |
dc.subject | kekerasan permukaan | en_US |
dc.title | Pengaruh Penambahan Zirkonium Oksida pada Restorasi Sementara Resin Akrilik Polimerisasi Panas pada Gigi Tiruan Cekat terhadap Kekuatan Fleksural dan Kekerasan Permukaan | en_US |
dc.type | Thesis | en_US |
dc.identifier.nim | NIM147160008 | |
dc.description.pages | 127 Halaman | en_US |
dc.description.type | Tesis Magister | en_US |